Stainless Steel Pipe for Chemical Processing: Grade Selection
Chlorides set the grade and acids refine it: 316L, 2205 and 904L compared by PREN, acid duty and temperature, plus the NDT and MTC clauses to specify.
By Dakai Steel Technical Team

Grade selection for chemical process piping starts with the medium. Two parameters decide most cases: which acid is present and at what concentration, and how much chloride the stream carries at what temperature. Below are the numbers for 316L, 2205 and 904L, the three grades that cover most chemical duty, plus the documents to put in the order.
The chloride question
Chlorides break down the passive film locally, and the three failure modes have separate thresholds. Pitting starts at inclusions and surface defects. Crevice corrosion starts under gaskets, weld spatter and support contacts where the solution stagnates. Chloride stress corrosion cracking needs austenite, tensile stress and temperature, and above roughly 60 C it becomes the governing limit for 300-series austenitics. Duplex and super-austenitic grades raise all three thresholds, but not equally. Rank candidates by PREN, then check the service temperature against measured critical pitting temperature.
Acids: which grade for which
Sulphuric and phosphoric acid, dilute and at ambient to moderate temperature, are 316L duty: the grade holds up to about 70% H2SO4 at room temperature and in dilute phosphoric acid to about 80 C, provided chlorides and fluorides are low. Hydrochloric acid removes 316L from consideration at any meaningful concentration; 904L is the practical starting point, and above roughly 60 C or in concentrated HCl the correct answer is a nickel alloy such as C-276. Nitric acid runs the other way: it is oxidising and chloride-free, so 304L is the standard choice and molybdenum adds cost without benefit.
316L versus 2205 versus 904L
316L (UNS S31603, EN 1.4404) carries 2.0-3.0% Mo with 16-18% Cr and 10-14% Ni at 0.030% C max; PREN is roughly 24-26. 2205 (UNS S32205, EN 1.4462) is duplex at 22% Cr, 3.0-3.5% Mo and 0.14-0.20% N, PREN 34-38, with 450 MPa minimum yield, about twice that of 316L. 904L (UNS N08904, EN 1.4539) is super-austenitic at 4.0-5.0% Mo and 23-28% Ni with 1.0-2.0% Cu, PREN about 34-36; the nickel and copper are there for reducing-acid service.
Select on the medium, not the ranking. 316L is the lowest-cost grade that holds clean, dilute acid duty, and it remains the right choice while chlorides stay below roughly 200 mg/L and the wall temperature below about 60 C. 2205 is the upgrade where chlorides are present and pressure or weight matters: the higher strength allows a thinner wall, and PREN 34-38 roughly doubles the chloride tolerance. 904L is the acid answer rather than the chloride answer, and the two are not interchangeable; confirm either against the alloy supplier's iso-corrosion diagram for the actual concentration and temperature.
PREN and temperature
PREN = %Cr + 3.3(%Mo + 0.5%W) + 16%N ranks alloys for pitting initiation and should be calculated from the heat analysis, not the grade minimums. A 316L heat at 17.2% Cr, 2.4% Mo and 0.04% N gives about 25.1; a 2205 heat at 22.5% Cr, 3.3% Mo and 0.17% N gives about 37.5. PREN contains no temperature term, which is where most selections fail: critical pitting temperature falls as chloride concentration rises, so the margin has to grow as the service gets hotter. Require CPT measured to ASTM G48 practice A or B and keep at least 15-20 C between service temperature and CPT.
What to specify
Fix five items in the order. Standard and grade: ASTM A312 or A213, or EN 10216-5, with the UNS or EN number beside the common name so substitution is visible. Chemistry: heat analysis on the certificate, plus a minimum PREN where chlorides are the reason for the grade. NDT: hydrostatic test to the standard pressure, then eddy current for tube or ultrasonic examination of wall and seam with the acceptance criteria named. Heat treatment: solution annealing temperature and cooling rate for 2205, which set ferrite balance. Documentation: EN 10204 3.1 mill test certificate as the baseline, 3.2 where an independent witness is required.
Send the medium, its concentration, the chloride level, design temperature and pressure, and we will return the grade, wall thickness and test schedule for comparison.